CoexFlex 30D TPE print settings
Print CoexFlex 30D TPE with a 220–240°C nozzle, a 25–85°C bed and the fan at 0–40%, with no enclosure, and dry it at 50°C for 4–6 hours.
These are COEX 3D's recommended starting settings, made to match the COEX 3D filament settings tables for every filament we make in Green Bay, Wisconsin. Treat each value as a starting point and adjust it for your printer.
1. Material notes
- Keep filament dry: store it sealed, and dry it again only after the spool has been exposed to air
- Dry an opened spool at 50°C for 4–6 hours
- No enclosure is needed
- Preferably use a direct drive extruder
- Print multiple parts one at a time (sequentially) to minimize stringing
- Use maximum travel speed to minimize stringing
2. Temperature settings
Nozzle temperature: 220–240°C
Bed temperature: 25–85°C
- Use a glue stick or hairspray as a release agent, or WELD3D. CoexFlex bonds very strongly to glass and smooth PEI, so a release agent protects both the print and the plate
3. Basic parameters
Unlike rigid filaments, TPE stretches as it is extruded and lays down thinner lines, so the line widths below are slightly smaller than the nozzle diameter. This keeps walls and perimeters properly bonded.
| Nozzle | Layer height | Line width | Max volumetric speed | Nozzle temperature |
|---|---|---|---|---|
| 0.4mm | 0.2mm | 0.35mm | 2.5 mm³/s | 240°C |
| 0.6mm | 0.3mm | 0.55mm | 5.6 mm³/s | 240°C |
| 0.8mm | 0.4mm | 0.75mm | 10.0 mm³/s | 240°C |
| 1.0mm | 0.5mm | 0.95mm | 15.6 mm³/s | 240°C |
4. Speed settings
0.4mm nozzle (max volumetric speed 2.5 mm³/s)
| Line type | Percentage | Speed |
|---|---|---|
| External perimeter | 50% | 17.86 mm/s |
| Internal perimeters | 75% | 26.79 mm/s |
| Infill | 100% | 35.71 mm/s |
| Top/bottom | 60% | 21.43 mm/s |
| First layer | 30% | 10.71 mm/s |
0.6mm nozzle (max volumetric speed 5.6 mm³/s)
| Line type | Percentage | Speed |
|---|---|---|
| External perimeter | 50% | 17.00 mm/s |
| Internal perimeters | 75% | 25.50 mm/s |
| Infill | 100% | 34.00 mm/s |
| Top/bottom | 60% | 20.40 mm/s |
| First layer | 30% | 10.20 mm/s |
0.8mm nozzle (max volumetric speed 10.0 mm³/s)
| Line type | Percentage | Speed |
|---|---|---|
| External perimeter | 50% | 16.67 mm/s |
| Internal perimeters | 75% | 25.00 mm/s |
| Infill | 100% | 33.33 mm/s |
| Top/bottom | 60% | 20.00 mm/s |
| First layer | 30% | 10.00 mm/s |
1.0mm nozzle (max volumetric speed 15.6 mm³/s)
| Line type | Percentage | Speed |
|---|---|---|
| External perimeter | 50% | 16.42 mm/s |
| Internal perimeters | 75% | 24.63 mm/s |
| Infill | 100% | 32.84 mm/s |
| Top/bottom | 60% | 19.70 mm/s |
| First layer | 30% | 9.85 mm/s |
5. Retraction settings
Important: Set travel speed to the maximum your machine allows (200–500mm/s). Faster moves give the filament less time to ooze, which reduces stringing.
| Nozzle | Distance | Speed | Z-hop |
|---|---|---|---|
| 0.4mm | 1.8–2.8mm | 35mm/s | 0.2mm |
| 0.6mm | 1.8–2.8mm | 35mm/s | 0.2mm |
| 0.8mm | 2.0–3.0mm | 35mm/s | 0.2mm |
| 1.0mm | 2.0–3.0mm | 35mm/s | 0.2mm |
6. Cooling settings
Cooling configuration:
- First layer: 0% (fan off)
- General printing: 0% (fan off)
- Force fan speed for overhangs and bridges: off
- Layers under 20 seconds: 40% fan speed