COEX ASA Prime print settings

Print ASA Prime with a 240–265°C nozzle, a 90–110°C bed and an enclosure, with little or no part cooling, and dry it at 80°C for 4–6 hours.

These are COEX 3D's recommended starting settings, made to match the COEX 3D filament settings tables for every filament we make in Green Bay, Wisconsin. Treat each value as a starting point and adjust it for your printer.

1. Material notes

  • Keep filament dry: store it sealed, and dry it again only after the spool has been exposed to air
  • Dry an opened spool at 80°C for 4–6 hours
  • An enclosure is required
  • Use a Z-offset slightly higher than for PLA (+0.05mm)
  • Enable "Avoid crossing perimeters" to reduce stringing
  • Consider using the "Wipe while retract" option
  • Enable "Slow down for small perimeters"
  • Print outer walls slower for better quality
  • Use a minimum layer time of 30 seconds for small parts
  • Consider using "Extra Prime Amount" after retraction

2. Temperature settings

Nozzle temperature: 240–265°C

Bed temperature: 90–110°C

  • Wash the bed often for good adhesion: use dish soap and rinse thoroughly to remove oils
  • Bed adhesion: use WELD3D or ABS/ASA slurry
  • Use a brim for tall or large prints
  • Keep the ambient temperature stable

3. Basic parameters

COEX ASA Prime basic parameters by nozzle size
Nozzle Layer height Line width Max volumetric speed Nozzle temperature
0.4mm 0.2mm 0.42mm 14.0 mm³/s 250°C
0.6mm 0.3mm 0.62mm 31.5 mm³/s 255°C
0.8mm 0.4mm 0.82mm 56.0 mm³/s 260°C
1.0mm 0.5mm 1.02mm 87.5 mm³/s 265°C

4. Speed settings

0.4mm nozzle (max volumetric speed 14.0 mm³/s)

COEX ASA Prime speeds for a 0.4mm nozzle
Line type Percentage Speed
External perimeter 50% 83.33 mm/s
Internal perimeters 75% 125.00 mm/s
Infill 100% 166.67 mm/s
Top/bottom 60% 100.00 mm/s
First layer 30% 50.00 mm/s

0.6mm nozzle (max volumetric speed 31.5 mm³/s)

COEX ASA Prime speeds for a 0.6mm nozzle
Line type Percentage Speed
External perimeter 50% 84.68 mm/s
Internal perimeters 75% 127.02 mm/s
Infill 100% 169.35 mm/s
Top/bottom 60% 101.61 mm/s
First layer 30% 50.81 mm/s

0.8mm nozzle (max volumetric speed 56.0 mm³/s)

COEX ASA Prime speeds for a 0.8mm nozzle
Line type Percentage Speed
External perimeter 50% 85.37 mm/s
Internal perimeters 75% 128.05 mm/s
Infill 100% 170.73 mm/s
Top/bottom 60% 102.44 mm/s
First layer 30% 51.22 mm/s

1.0mm nozzle (max volumetric speed 87.5 mm³/s)

COEX ASA Prime speeds for a 1.0mm nozzle
Line type Percentage Speed
External perimeter 50% 85.78 mm/s
Internal perimeters 75% 128.68 mm/s
Infill 100% 171.57 mm/s
Top/bottom 60% 102.94 mm/s
First layer 30% 51.47 mm/s

5. Retraction settings

Important: Set travel speed to the maximum your machine allows (200–500mm/s). Faster moves give the filament less time to ooze, which reduces stringing.

COEX ASA Prime retraction by nozzle size
Nozzle Distance Speed Z-hop
0.4mm 1.0–1.5mm 40mm/s 0.2mm
0.6mm 1.0–1.5mm 40mm/s 0.2mm
0.8mm 1.0–1.5mm 40mm/s 0.2mm
1.0mm 1.0–1.5mm 40mm/s 0.2mm

6. Cooling settings

Cooling configuration:

  • First layer: 0% (fan off)
  • General printing: little or no part cooling
  • Bridges and overhangs: low fan speed only
  • Layers under 15 seconds: low fan speed only

7. Troubleshooting

COEX ASA Prime troubleshooting
Problem Solution
Irregular extrusion
  1. Dry the filament
  2. Check the extruder
  3. Reduce speed
Poor adhesion
  1. Dry the filament
  2. Use an adhesive
  3. Adjust the first layer
Stringing
  1. Dry the filament
  2. Adjust retraction
  3. Increase travel speed
  4. Check temperature

Please note: These printing parameters are initial recommendations based on our experience. They may need adjustment for your specific 3D printer, environmental conditions and the geometry of the part you are printing. Use them as a starting point and fine-tune them for your needs.